C276

Category:Hastelloy alloy

Name:C276

Main products:Plate, rod, tube, strip, wire, etc

Product hotline:008613812088888

Introduction

This alloy exhibits excellent corrosion resistance to most corrosive media in both oxidation and reduction states. Excellent resistance to point corrosion, crevice corrosion, and stress corrosion cracking. Alloy is suitable for various chemical process industries containing oxidizing and reducing media. The higher content of molybdenum and chromium makes the alloy resistant to chloride ion erosion, and the tungsten element further improves its corrosion resistance. Hastelloy C-276 is one of the few materials that can withstand corrosion from moisture, hypochlorite, and chlorine dioxide solutions. This alloy exhibits significant corrosion resistance to high concentrations of chloride solutions, such as iron chloride and copper chloride.

Hastelloy C-276 Chemical composition:

               

合金 牌号

%


Ni


Cr

铁 
Fe

钼 
Mo


W

钴 
Co

碳 
C

锰 
Mn

硅 
Si

硫 
S

磷 
P

钒 
V

钛 
Ti

HastelloyC-276

Min

余量

15.0

4.0

15.0

3.0







0.1


Max

16.5

7.0

17.0

4.5

2.5

0.01

1.0

0.08

0.001

0.015

0.3





 

Hastelloy C-276物理性能:









密度 
g/cm3

熔点 

热导率 
λ/(W/m•℃)

比热容 
J/kg•℃

弹性模量 
GPa

剪切模量 
GPa

电阻率 
μΩ•m

泊松比

线膨胀系数 
a/10-6℃-1

8.9

1325~1370

10.2(100℃)

407

208

79

1.25


11.7(20~100℃)


 

Hastelloy C-276力学性能:(在20℃检测机械性能的最小值)





热处理方式

抗拉强度σb/MPa

屈服强度σp0.2/MPa

延伸率σ5 /%

布氏硬度 HBS

固溶处理

758

363

62



Hastelloy C-276生产执行标准:





标准

棒材

锻件

板(带)材

管材

美国材料与试验协会

ASTM  B574

ASTM  B564

ASTM  B575

ASTM  B622

ASTM  B619

ASTM  B626

美国机械工程师协会

ASME  SB574

ASME  SB564

ASME  SB575

ASTM  SB622

ASTM  SB619

ASTM  SB626


Hastelloy C-276金相组织结构:

合金为为面心立方晶格结构。

Hastelloy C-276工艺性能与要求:

1、热加工燃料中的含硫量越低越好,天然气中的硫含量应少于0.1%,重油中硫含量应少于0.5%。

2、合金的热加工温度范围1200℃~950℃,冷却方式为水冷或快速空冷。

3、适合采用任何传统焊接工艺焊接,如钨电极惰性气体保护焊、等离子弧焊、手工亚弧焊、金属极惰性气体保护焊、熔化极惰性气体保护焊。


 